Prima Creator PrimaSelect Glow in the Dark PLA Glow Green
Material Engineering Report MaterialID MAT0128
3DPIceland Engineering Platform 3DPIceland Labs Generated with 3DPIceland Engineering Platform v70.0.4 DIRECT-IMPACT-METHODOLOGY - Izod and Charpy Methodology Generated 2026-10-04 18:07:33
Public-data contract: This static report contains only allowlisted material identity, public links, canonical MSRP and existing Verified Material Summary / governed score outputs. It excludes raw specimen rows and non-public operational data.
Prima Creator PrimaSelect Glow in the Dark PLA Glow Green
Manufacturer
Prima Creator
Product line
PrimaSelect
Base material
PLA
Category
Standard
Variant / finish
Glow
Reinforcement
—
Color
Green
Governed engineering profile
Overall
—
Tensile
27/100
Impact
—
Izod
—
Charpy
—
Stiffness
72/100
Consistency
70/100
Layer adhesion
18/100
Thermal
26/100
Best available axis
stiffness
Engineering score profile
Overall
—
Tensile
27/100
Impact
—
Izod
—
Charpy
—
Stiffness
72/100
Consistency
70/100
Layer adhesion
18/100
Thermal
26/100
Engineering radar
Selected material
Material average - PLA
Manufacturer average - Prima Creator
Legacy Impact radar: 20.535 % of legacy rig capacity. This historical visual reference is the mean corrected Flat/Upright result divided by the matching rig capacity; it is not a modern engineering score.
Izod and Charpy use versioned method references and together form one equally weighted impact family. Overall requires all five families and both calibrated methods; incomplete profiles are not ranked. Legacy Impact and thermal are outside Overall. Missing axes have gaps with no marker or filled polygon; measured zero retains a centre marker.
Fixture thermal result
51 °C · score 26/100 · method 3dp-thermal-deflection-fixture-v1 Nearby BlueDOT probe-indicated fixture temperature from a non-standard comparative 3DPIceland method; not ASTM D648, ISO 75, specimen temperature, certified HDT or a manufacturer limit.
Material and manufacturer context
Metric
Selected material
Material average
Manufacturer average
Overall
—
—
—
Tensile
27/100
30/100
27/100
Impact
—
—
—
Izod
—
8/100
8/100
Charpy
—
10/100
8/100
Stiffness
72/100
87/100
76/100
Consistency
70/100
75/100
71/100
Layer adhesion
18/100
31/100
22/100
Thermal
26/100
—
—
Verified measurement results
Existing Verified Material Summary outputs. The public renderer does not read raw specimen rows or recalculate these values.
Measurement
Average
Std. deviation
CV
Samples
Confidence
Tensile upright
6.475 MPa
3.195 MPa
49.3%
10
10/10
Tensile flat
36.176 MPa
3.55 MPa
9.8%
10
10/10
Impact upright
7.113 kJ/m²
1.669 kJ/m²
23.5%
10
10/10
Impact flat
16.285 kJ/m²
0.912 kJ/m²
5.6%
10
10/10
Izod
—
—
—
—
—
Charpy
—
—
—
—
—
Stiffness modulus
2170.732 MPa
—
—
—
—
Stiffness deflection
2.5 mm
—
—
—
—
Measurement provenance
Canonical per-module measured dates from SQLite, shown in unambiguous ISO format. Missing dates are not inferred.
Module
Measured date
Tensile
2026-07-24
Impact
Not recorded
Izod
Not recorded
Charpy
Not recorded
Stiffness
Not recorded
Thermal
Not recorded
Engineering interpretation
Summary: Prima Creator PrimaSelect Glow in the Dark PLA Glow Green has a profile awaiting complete scoring evidence. It is without enough material-family average context and without enough manufacturer average context. Its strongest measured axis is Stiffness, while the weakest axis is Layer Adhesion.
Data-driven review: Prima Creator PrimaSelect Glow in the Dark PLA Glow Green has incomplete scoring evidence or pending method references. Overall suitability and ranking are unavailable. Available scored axes can be inspected separately; missing scores do not establish weak material performance.
Best feature
Stiffness
Main limitation
Layer Adhesion
Dataset position
—
—
Strengths
Consistency: 70/100. Repeatability is one of the stronger signals in this material profile.
Stiffness: 72/100. Stiffness is a relative advantage in this comparison group.
Limitations
Tensile: 27/100. Avoid using this as the primary choice for tensile-loaded parts.
Stiffness: 72/100. Expect less shape stability than the stronger materials in the same family.
Layer adhesion: 18/100. Z-axis performance should be treated with caution.
Engineering trade-offs
Good repeatability does not compensate for low tensile capability in load-bearing designs.
Recommended applications
Rigid brackets, fixtures and shape-stable prototypes
Repeatable print jobs and production-style batches
Cosmetic parts, concept models or low-load prototypes
Avoid high tensile load applications
Metric rankings and percentiles
Metric
Score
Rank
Percentile
Overall
—
—
—
Tensile
27/100
142 / 243
Better than 42%
Impact
—
—
—
Izod
—
—
—
Charpy
—
—
—
Stiffness
72/100
144 / 240
Better than 40%
Consistency
70/100
170 / 243
Better than 30%
Layer adhesion
18/100
158 / 243
Better than 35%
Thermal
26/100
190 / 226
Better than 16%
Decision guidance
Overall suitability is unavailable until the required measurements and method references are complete.
Do not choose it as a tensile-strength benchmark material.
Better alternatives
MaterialID
Material
Manufacturer
Overall
Tensile
Impact
Izod
Charpy
No stronger same-base-material alternatives were identified in the current governed dataset.
Peer context
Highest-scoring same-base-material peers from the current governed dataset. This context is descriptive and is not recalculated by the public renderer.
Results are comparative 3DPIceland measurements from home-built test equipment. Thermal is a nearby BlueDOT probe-indicated fixture temperature, not ASTM D648, ISO 75 or specimen temperature. Missing evidence remains n/a. Scores and test results are not recalculated by this publishing layer and do not replace certified manufacturer datasheets or accredited laboratory testing.