Public engineering report

Eryone Standard White ASA White

Material Engineering Report
MaterialID MAT0216
3DPIceland Engineering Platform
3DPIceland Labs
Generated with 3DPIceland Engineering Platform v70.0.4 DIRECT-IMPACT-METHODOLOGY - Izod and Charpy Methodology
Generated 2026-10-04 18:07:33
Public-data contract: This static report contains only allowlisted material identity, public links, canonical MSRP and existing Verified Material Summary / governed score outputs. It excludes raw specimen rows and non-public operational data.
Rigid test coverage
Partial; 4/5 score families; Izod/Charpy 0/2 measured, 0/2 scored; Overall unavailable: missing measurements or references; policy engineering-score-v70-1
Engineering axes
5/8
Public MSRP
$15.00 USD/kg

Material identity

MaterialIDMAT0216
MaterialEryone Standard White ASA White
ManufacturerEryone
Product lineStandard
Base materialASA
CategoryEngineering
Variant / finish—
Reinforcement—
ColorWhite

Governed engineering profile

Overall—
Tensile23/100
Impact—
Izod—
Charpy—
Stiffness71/100
Consistency70/100
Layer adhesion8/100
Thermal45/100
Best available axisstiffness

Engineering score profile

Overall
—
Tensile
23/100
Impact
—
Izod
—
Charpy
—
Stiffness
71/100
Consistency
70/100
Layer adhesion
8/100
Thermal
45/100

Engineering radar

TensileLegacy Impact %IzodCharpyStiffnessThermalLayer adhesionConsistency
Selected material
Material average - ASA
Manufacturer average - Eryone

Legacy Impact radar: 43.465 % of legacy rig capacity. This historical visual reference is the mean corrected Flat/Upright result divided by the matching rig capacity; it is not a modern engineering score.

Izod and Charpy use versioned method references and together form one equally weighted impact family. Overall requires all five families and both calibrated methods; incomplete profiles are not ranked. Legacy Impact and thermal are outside Overall. Missing axes have gaps with no marker or filled polygon; measured zero retains a centre marker.

Fixture thermal result

89 °C · score 45/100 · method 3dp-thermal-deflection-fixture-v1
Nearby BlueDOT probe-indicated fixture temperature from a non-standard comparative 3DPIceland method; not ASTM D648, ISO 75, specimen temperature, certified HDT or a manufacturer limit.

Material and manufacturer context

MetricSelected materialMaterial averageManufacturer average
Overall———
Tensile23/10019/10024/100
Impact———
Izod—17/10016/100
Charpy—30/10018/100
Stiffness71/10068/10073/100
Consistency70/10071/10070/100
Layer adhesion8/10020/10021/100
Thermal45/100——

Verified measurement results

Existing Verified Material Summary outputs. The public renderer does not read raw specimen rows or recalculate these values.

MeasurementAverageStd. deviationCVSamplesConfidence
Tensile upright2.725 MPa1.16 MPa42.6%77/10
Tensile flat34.094 MPa3.872 MPa11.4%99/10
Impact upright5.02 kJ/m²1.368 kJ/m²27.3%1010/10
Impact flat44.507 kJ/m²1.365 kJ/m²3.1%1010/10
Izod—————
Charpy—————
Stiffness modulus2120.83 MPa————
Stiffness deflection2.559 mm————

Measurement provenance

Canonical per-module measured dates from SQLite, shown in unambiguous ISO format. Missing dates are not inferred.

ModuleMeasured date
Tensile2026-07-31
Impact2026-08-01
IzodNot recorded
CharpyNot recorded
Stiffness2026-07-31
ThermalNot recorded

Engineering interpretation

Summary: Eryone Standard White ASA White has a profile awaiting complete scoring evidence. It is without enough material-family average context and without enough manufacturer average context. Its strongest measured axis is Stiffness, while the weakest axis is Layer Adhesion.
Data-driven review: Eryone Standard White ASA White has incomplete scoring evidence or pending method references. Overall suitability and ranking are unavailable. Available scored axes can be inspected separately; missing scores do not establish weak material performance.
Best feature
Stiffness
Main limitation
Layer Adhesion
Dataset position
—
—

Strengths

  • Consistency: 70/100. Repeatability is one of the stronger signals in this material profile.
  • Stiffness: 71/100. Stiffness is a relative advantage in this comparison group.

Limitations

  • Tensile: 23/100. Avoid using this as the primary choice for tensile-loaded parts.
  • Layer adhesion: 8/100. Z-axis performance should be treated with caution.

Engineering trade-offs

  • Good repeatability does not compensate for low tensile capability in load-bearing designs.

Recommended applications

  • Rigid brackets, fixtures and shape-stable prototypes
  • Repeatable print jobs and production-style batches
  • Cosmetic parts, concept models or low-load prototypes
  • Avoid high tensile load applications

Metric rankings and percentiles

MetricScoreRankPercentile
Overall———
Tensile23/100173 / 243Better than 29%
Impact———
Izod———
Charpy———
Stiffness71/100153 / 240Better than 37%
Consistency70/100174 / 243Better than 29%
Layer adhesion8/100233 / 243Better than 5%
Thermal45/10027 / 226Better than 88%

Decision guidance

Better alternatives

MaterialIDMaterialManufacturerOverallTensileImpactIzodCharpy
No stronger same-base-material alternatives were identified in the current governed dataset.

Peer context

Highest-scoring same-base-material peers from the current governed dataset. This context is descriptive and is not recalculated by the public renderer.

MaterialIDMaterialManufacturerOverallTensileImpactIzodCharpy
MAT0015Prusa3D Prusament ASA Pro GreenPrusa3D48/10023/100—n/an/a
MAT0197Siraya Tech Fiberheart Black ASA GF BlackSiraya Tech43/10021/100—n/an/a
MAT0010Yasin Standard Black ASA GF BlackYasin42/10021/100—n/an/a
MAT0012Prusa3D Prusament Galaxy Black ASA BlackPrusa3D41/10018/100—n/an/a
MAT0218Eryone Standard White ASA GF WhiteEryone40/10017/100—n/an/a
MAT0011Extrudr DuraPro Neon Green ASA GF GreenExtrudr40/10015/100—n/an/a
MAT0009Yasin Standard Black ASA CF BlackYasin40/10020/100—n/an/a
MAT0008Extrudr DuraPro ASA CF BlackExtrudr39/10015/100—n/an/a

Public links

Methodology and limitations

Results are comparative 3DPIceland measurements from home-built test equipment. Thermal is a nearby BlueDOT probe-indicated fixture temperature, not ASTM D648, ISO 75 or specimen temperature. Missing evidence remains n/a. Scores and test results are not recalculated by this publishing layer and do not replace certified manufacturer datasheets or accredited laboratory testing.