Public test session report

Prusa3D Prusament Marble Gray PLA Marble Gray

MaterialID MAT0205

3DPIceland Labs
Generated with 3DPIceland Engineering Platform v70.0.4 DIRECT-IMPACT-METHODOLOGY - Izod and Charpy Methodology
2026-10-04 18:10:39

Traceability boundary: canonical per-module measured dates are shown below. Session identifier, time of day, operator, printer/slicer profile and environmental conditions are Not recorded and are never inferred.

Measurement provenance

Canonical SQLite measured dates use ISO format; missing dates remain Not recorded.

ModuleMeasured date
TensileNot recorded
Impact2026-07-30
Izod2026-09-30
Charpy2026-09-30
StiffnessNot recorded
Rigid test status
Complete
Rigid result modules
6/6
Rigid specimen/result records
41
Public details
Approved

Rigid specimen and result quality

ModuleOrientationAverageStd. dev.CVSpecimensConfidenceValidation
TensileUpright14,366 MPa6,421 MPa0,447%1010/10OK
TensileFlat45,066 MPa6,506 MPa0,144%1010/10OK
ImpactUpright6,494 kJ/m²0,822 kJ/m²0,127%1010/10OK
ImpactFlat10,786 kJ/m²0,623 kJ/m²0,058%1010/10OK
StiffnessThree-point bend3181,245 MPan/an/a1CompleteOK

Recorded native inputs

ModuleInput setRecorded values
TensileUpright force inputs (N)75, 86, 22, 144, 90, 68, 154, 124, 52, 119
TensileFlat force inputs (N)278, 309, 253, 344, 343, 321, 220, 305, 245, 312
ImpactUpright needle inputs (%)8,5, 7, 8, 7,5, 9, 9, 6,5, 7, 9,5, 8
ImpactFlat needle inputs (%)14, 12, 14, 12, 13, 13,5, 14, 13,5, 13, 13
StiffnessRevolutions / degrees1 / 220

Approved test notes

Method and equipment context

Purpose-built tensile, pendulum impact and three-point bend apparatus are used with the governed Settings Manager constants consumed by ResultsService. Results are comparative and do not claim accredited-laboratory equipment.

Testing methodology · Engineering methodology whitepaper · Download PDF

Izod and Charpy Impact Strength

Izod Impact Strength · 2026-09-30
Instrument readings in kJ/m²
Mean 3.807 kJ/m²; Std. Dev 0.086 kJ/m²; CV 2.272%; Samples 10; Confidence 10
No break 0; invalid 0; excluded 0.
Comparative measurements; standard conformity unverified.

Charpy Impact Strength · 2026-09-30
Instrument readings in kJ/m²
Mean 3.556 kJ/m²; Std. Dev 0.435 kJ/m²; CV 12.243%; Samples 10; Confidence 10
No break 0; invalid 0; excluded 0.
Comparative measurements; standard conformity unverified.