Public test session report

Eryone Standard Black PA6 GF Black

MaterialID MAT0210

3DPIceland Labs
Generated with 3DPIceland Engineering Platform v70.0.4 DIRECT-IMPACT-METHODOLOGY - Izod and Charpy Methodology
2026-10-04 18:10:39

Traceability boundary: canonical per-module measured dates are shown below. Session identifier, time of day, operator, printer/slicer profile and environmental conditions are Not recorded and are never inferred.

Measurement provenance

Canonical SQLite measured dates use ISO format; missing dates remain Not recorded.

ModuleMeasured date
Tensile2026-09-14
Impact2026-08-02
Izod2026-09-30
Charpy2026-09-30
Stiffness2026-08-01
Rigid test status
Complete
Rigid result modules
6/6
Rigid specimen/result records
39
Public details
Approved

Rigid specimen and result quality

ModuleOrientationAverageStd. dev.CVSpecimensConfidenceValidation
TensileUpright4,23 MPa2,995 MPa0,708%88/10OK
TensileFlat58,355 MPa9,191 MPa0,158%1010/10OK
ImpactUpright5,06 kJ/m²1,236 kJ/m²0,244%1010/10OK
ImpactFlat33,509 kJ/m²2,276 kJ/m²0,068%1010/10OK
StiffnessThree-point bend3181,245 MPan/an/a1CompleteOK

Recorded native inputs

ModuleInput setRecorded values
TensileUpright force inputs (N)23, 6, 40, 11, 60, 48, 17, 15, ,
TensileFlat force inputs (N)439, 416, 342, 441, 332, 416, 258, 398, 417, 335
ImpactUpright needle inputs (%)3, 7, 8, 5,5, 6, 6, 8, 5, 7, 7
ImpactFlat needle inputs (%)41, 49, 41, 42, 40, 38, 44, 44, 39, 40
StiffnessRevolutions / degrees1 / 220

Approved test notes

Method and equipment context

Purpose-built tensile, pendulum impact and three-point bend apparatus are used with the governed Settings Manager constants consumed by ResultsService. Results are comparative and do not claim accredited-laboratory equipment.

Testing methodology · Engineering methodology whitepaper · Download PDF

Izod and Charpy Impact Strength

Izod Impact Strength · 2026-09-30
Instrument readings in kJ/m²
Mean 19.164 kJ/m²; Std. Dev 5.524 kJ/m²; CV 28.823%; Samples 10; Confidence 10
No break 0; invalid 0; excluded 0.
Comparative measurements; standard conformity unverified.

Charpy Impact Strength · 2026-09-30
Instrument readings in kJ/m²
Mean 18.38 kJ/m²; Std. Dev 0.917 kJ/m²; CV 4.987%; Samples 10; Confidence 10
No break 0; invalid 0; excluded 0.
Comparative measurements; standard conformity unverified.